LOSTWAXTRInvestment Casting

GX2CrNiMo19-11-2 (1.4409) — Low-carbon Mo-bearing austenitic stainless steel, cast 316L type

Designation

Grade
GX2CrNiMo19-11-2 (1.4409)
UNS
—
EN designation
1.4409 (GX2CrNiMo19-11-2)
Standard
EN 10283
Density
≈ 7.75 g/cm³
Usual delivery condition
Solution annealed and quenched

Chemical composition

ElementMass fraction, %
C≤ 0.030
Mn≤ 2.00
Si≤ 1.50
Cr18.0–20.0
Ni9.0–12.0
Mo2.0–2.5
N≤ 0.20
Febal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Solution annealed and quenched44019530

Minimum values (or ranges) for separately cast test bars as specified in EN 10283.

Characteristics

Corrosion and oxidation behaviour
Good general resistance with improved resistance to chloride pitting through molybdenum
Weldability
Good with matching filler and standard procedures
Machinability
Moderate; work hardening or built-up edge to be considered
Typical applications
Valves Pumps Marine Chemical processing Food processing

International cross-reference

SystemDesignationRelationship
ASTMCF3M (ASTM A351/A351M, A743/A743M)Similar composition
EN (wrought)1.4404 (X2CrNiMo17-12-2)Comparable properties

Casting and processing considerations

Castings are normally solution annealed and rapidly cooled to dissolve carbides and restore corrosion resistance. Low-carbon grades are preferred where castings will be welded without subsequent heat treatment. High shrinkage requires adequate feeding of heavy sections; surface finish and pickling or passivation requirements should be agreed in advance.

Reference data compiled from the cited standards for orientation. Always work from the current edition of the governing specification; values are not a guaranteed LOSTWAX TR delivery specification.

CF8 GX5CrNi19-10 (1.4308) CF3 GX2CrNi19-11 (1.4309) CF8M GX5CrNiMo19-11-2 (1.4408) CF3M CN7M CK3MCuN