CD4MCuN (1B) — 25Cr duplex stainless steel with copper

Designation

Grade
CD4MCuN (1B)
UNS
J93372
EN designation
—
Commonly associated designations
Ferralium® 255 type
Type designations and trade names are given for orientation only. Trade names are trademarks of their respective owners; the cast grade and its standard remain the specification.
Standard
ASTM A890/A890M, A995/A995M
Density
≈ 7.80 g/cm³
Usual delivery condition
Solution annealed and quenched

Chemical composition

ElementMass fraction, %
C≤ 0.04
Mn≤ 1.0
Si≤ 1.0
Cr24.5–26.5
Ni4.7–6.0
Mo1.7–2.3
Cu2.7–3.3
N0.10–0.25
Febal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Solution annealed and quenched69048516

Minimum values (or ranges) for separately cast test bars as specified in ASTM A890/A890M, A995/A995M.

Characteristics

Corrosion and oxidation behaviour
High resistance to chloride pitting, crevice and stress corrosion cracking
Weldability
Possible with qualified procedure; preheat and/or post-weld heat treatment as specified
Machinability
Difficult; rigid set-ups, low cutting speeds or grinding
Typical applications
Valves Pumps Offshore Marine Chemical processing

International cross-reference

Casting and processing considerations

The phase balance and freedom from intermetallic phases such as sigma depend on a correct solution anneal followed by rapid quenching; slow cooling of heavy sections is the main risk. Ferrite content, impact toughness and corrosion testing are frequently specified as acceptance tests and should be defined at the enquiry stage.

Reference data compiled from the cited standards for orientation. Always work from the current edition of the governing specification; values are not a guaranteed LOSTWAX TR delivery specification.

CD3MN (4A) GX2CrNiMoN22-5-3 (1.4470) CE3MN (5A) GX2CrNiMoN26-7-4 (1.4469) CD3MWCuN (6A)