LOSTWAXTRInvestment CastingRequest a quotation

GX2NiCrMoCu25-20-5 (1.4584) — High-alloy austenitic stainless steel with Mo and Cu, cast 904L type

Designation

Grade
GX2NiCrMoCu25-20-5 (1.4584)
UNS
—
EN designation
1.4584 (GX2NiCrMoCu25-20-5)
Commonly associated designations
904L type (Uranus® B6)
Type designations and trade names are given for orientation only. Trade names are trademarks of their respective owners; the cast grade and its standard remain the specification.
Standard
EN 10283
Density
≈ 8.00 g/cm³
Usual delivery condition
Solution annealed and quenched

Chemical composition

ElementMass fraction, %
C≤ 0.025
Mn≤ 2.00
Si≤ 1.00
Cr19.0–21.0
Ni24.0–26.0
Mo4.0–5.0
Cu1.0–3.0
N≤ 0.20
Febal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Solution annealed and quenched45018530

Minimum values (or ranges) for separately cast test bars as specified in EN 10283.

Characteristics

Corrosion and oxidation behaviour
Selected for acids and aggressive chemical process media
Weldability
Possible with qualified procedure; preheat and/or post-weld heat treatment as specified
Machinability
Moderate; work hardening or built-up edge to be considered
Typical applications
Valves Pumps Chemical processing

International cross-reference

SystemDesignationRelationship
EN (wrought)1.4539 (X1NiCrMoCu25-20-5), UNS N08904 / 904LComparable properties

Casting and processing considerations

Castings are normally solution annealed and rapidly cooled to dissolve carbides and restore corrosion resistance. Low-carbon grades are preferred where castings will be welded without subsequent heat treatment. High shrinkage requires adequate feeding of heavy sections; surface finish and pickling or passivation requirements should be agreed in advance.

Reference data compiled from the cited standards for orientation. Always work from the current edition of the governing specification; values are not a guaranteed LOSTWAX TR delivery specification.

CF8 GX5CrNi19-10 (1.4308) CF3 CF8C GX2CrNi19-11 (1.4309) CF8M GX5CrNiMo19-11-2 (1.4408) CF3M GX2CrNiMo19-11-2 (1.4409) CG8M CN7M CK3MCuN CN3MN