LOSTWAXTRInvestment CastingRequest a quotation

CX2MW — Ni-Cr-Mo-W alloy, low carbon, cast C-22 type

Designation

Grade
CX2MW
UNS
N26022
EN designation
—
Commonly associated designations
Hastelloy® C-22 / C22 type
Type designations and trade names are given for orientation only. Trade names are trademarks of their respective owners; the cast grade and its standard remain the specification.
Standard
ASTM A494/A494M
Density
≈ 8.64 g/cm³
Usual delivery condition
Solution annealed and quenched

Chemical composition

ElementMass fraction, %
C≤ 0.02
Mn≤ 1.00
Si≤ 0.80
Cr20.0–22.5
Mo12.5–14.5
W2.5–3.5
Fe2.0–6.0
V≤ 0.35
Nibal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Solution annealed and quenched55031030

Minimum values (or ranges) for separately cast test bars as specified in ASTM A494/A494M.

Characteristics

Corrosion and oxidation behaviour
Selected for acids and aggressive chemical process media
Weldability
Good with matching filler and standard procedures
Machinability
Difficult; rigid set-ups, low cutting speeds or grinding
Typical applications
Valves Pumps Chemical processing

International cross-reference

SystemDesignationRelationship
UNS (wrought)N06022Comparable properties

Casting and processing considerations

Melting practice has a strong influence on quality: reactive elements such as aluminium and titanium in superalloys normally require vacuum melting and pouring, while corrosion-resistant grades are commonly air melted with careful control of carbon and silicon. Corrosion-resistant grades are solution annealed; weld repair and its heat treatment must follow the material specification.

Reference data compiled from the cited standards for orientation. Always work from the current edition of the governing specification; values are not a guaranteed LOSTWAX TR delivery specification.

CW-12MW CW-2M CW-6M N-7M CW-6MC CU5MCuC M-35-1 CY-40 CZ-100 Alloy 718