LOSTWAXTRInvestment CastingRequest a quotation

CU5MCuC — Ni-Fe-Cr-Mo-Cu alloy, Nb-stabilised, cast 825 type

Designation

Grade
CU5MCuC
UNS
N08826
EN designation
—
Commonly associated designations
Incoloy® 825 type
Type designations and trade names are given for orientation only. Trade names are trademarks of their respective owners; the cast grade and its standard remain the specification.
Standard
ASTM A494/A494M
Density
≈ 8.44 g/cm³
Usual delivery condition
Solution annealed and quenched

Chemical composition

ElementMass fraction, %
C≤ 0.050
Mn≤ 1.0
Si≤ 1.0
Cr19.5–23.5
Ni38.0–44.0
Mo2.5–3.5
Cu1.5–3.5
Nb0.60–1.20
Febal.

Main elements only. Phosphorus, sulphur and residual-element limits are specified in the standard and are not reproduced here.

Mechanical properties

ConditionTensile strength Rm, min. (MPa)Yield strength Rp0.2, min. (MPa)Elongation, min. (%)
Solution annealed and quenched52024020

Minimum values (or ranges) for separately cast test bars as specified in ASTM A494/A494M.

Characteristics

Corrosion and oxidation behaviour
Very good resistance in seawater and chloride-bearing media
Weldability
Good with matching filler and standard procedures
Machinability
Difficult; rigid set-ups, low cutting speeds or grinding
Typical applications
Valves Pumps Marine Offshore Chemical processing

International cross-reference

SystemDesignationRelationship
UNS (wrought)N08825Comparable properties

Casting and processing considerations

Melting practice has a strong influence on quality: reactive elements such as aluminium and titanium in superalloys normally require vacuum melting and pouring, while corrosion-resistant grades are commonly air melted with careful control of carbon and silicon. Corrosion-resistant grades are solution annealed; weld repair and its heat treatment must follow the material specification.

Reference data compiled from the cited standards for orientation. Always work from the current edition of the governing specification; values are not a guaranteed LOSTWAX TR delivery specification.

CW-12MW CW-2M CX2MW CW-6M N-7M CW-6MC M-35-1 CY-40 CZ-100 Alloy 718